Ethylene-vinyl acetate EVA Interlayer Film common problems

EXTERNAL SAFETY EVA interlayer Film

Analysis and solution to common problems
 ●Bubble
 1.) The plainness of the glass is poor (especially the tempered glass). Make sure the thickness of the inserted film is more than the deformation scale of the two overlapping glasses.
 2.) The film has not completely melted. Please raise the temperature or increase the time of heat-holding time!
 3.) Stop the vacuum pump two early. Don’t stop the vacuum pump until the temperature bellows 50℃.
 4.)The Silica Gel Bag is leaking. Please replace the Silica Gel Bag to unsure that the vacuum value reaches 0.095Mpa. 
 
 ●Degumming
1.) Processing temperature or heal-holding time(keeping that temperature) is not enough.
2.) The best working period for film is within 6 month. Please use the film within the period.
3.) The glass surface is not clean. Please clean the glass surface.

 ●Self-exposing
 1.) Please cool the glass gradually avoiding water.
 2.) Make sure the film you used has been improved by eliminated static and tension.
 If you need any help in China to find the informations of glass lamination materials,  products, manufacturers, Suppliers, Offers, Please feel free to contact us, we will answer you in 24hours.

Mail: helps@glasshelps.com

China GlassHepls Service Center of Glass Materials Purchase